A single S230 cast-steel shot is 0.58 mm across and weighs 0.80 mg. At 60 m/s it carries 1.44 mJ. It arrives at a steel surface, stays in contact for a few microseconds, and leaves a crater roughly 145 µm wide and 10–20 µm deep. If the contact stayed elastic, Hertz would put 18 GPa at the centre — about six times the 3σy limit of a 1 GPa steel. It does not stay elastic. The shot yields the surface, and the useful product is not the crater at all. It is the layer underneath: a skin of metal that was stretched plastically and is now held in compression by the elastic bulk behind it.
That layer is why a carburised gear that survived 9,850 cycles unpeened survived 33,167 cycles at the optimum intensity in one widely cited test — and why the same gear, peened harder at 8C, fell back to 16,375. Shot peening is not a finish. It is a fatigue-design input with a process window, and the window has a hard edge on both sides.
The difficulty is that the process is specified in a language that sounds like strength but is not. “8A” is not a pressure, a velocity, or a stress. It is the arc height of a sacrificial 1.29 mm steel strip at saturation, expressed in thousandths of an inch. “200% coverage” is not twice the area; it is twice the time needed to reach 98% physical coverage. Two shops can both claim 8A at 200% and produce different residual-stress profiles, because intensity is a property of the shot stream and coverage is a property of time, while the layer that actually protects the part depends on the material, the shot size, the angle, and what happened before and after peening.
This guide follows the chain from a single impact to a released drawing: contact mechanics, Almen arithmetic, coverage statistics, residual-stress profiles, over-peening, media and machine variables, fatigue data, additive manufacturing, weld toe treatment, peen forming, quality control, and cost.
1. What one impact leaves behind
Shot peening is a cold-working process. Each round particle strikes at normal incidence and plastically stretches a thin surface layer. When the shot rebounds, the deformed skin cannot contract back to its original length because the elastic core beneath it is still there. The result is a self-equilibrated stress field: compression in the surface layer, tension in the core, and a bending moment that is balanced through the thickness.
For a peened layer of depth t carrying a compressive stress \sigma_c, force balance through a plate of thickness H requires
and the balancing tensile stress in the unpeened core is approximately
For a 20 mm plate with a 0.3 mm layer at −600 MPa, the core tension is only about 9 MPa. That asymmetry is the point: a thin, highly stressed skin can be introduced without loading the whole section. It is also why thin parts distort. At H = 3 mm, the same layer produces about 67 MPa of balancing tension and enough bending moment to bow the part visibly.
The residual-stress profile is not a step function. It typically starts at a surface value of 0.4–0.6 of the yield strength, rises to a peak 20–75 µm below the surface, and crosses zero at 0.1–0.5 mm. The near-surface “hook” is characteristic of peening: the very surface has less constraint and partially relaxes, while the layer just below it carries the peak compression.
A representative measured profile is 18CrNiMo7-6 gear steel peened to full coverage: the compressive layer extends to about 0.4 mm, the peak compressive stress is −1,105 MPa at a depth of 0.07–0.075 mm, and raising coverage from 100% to 200% moves the peak only to −1,210 MPa without changing the layer thickness. Beyond 200%, the profile is essentially saturated. More peening does not buy a proportionally deeper layer; it buys surface damage.
The same impact also changes the microstructure. Dislocation density rises, grains near the surface refine, and the surface hardens. That cold work contributes to fatigue resistance, but it is not free: ductility near the surface falls, and the surface roughness rises. A peened surface is matte and dimpled, not cosmetic. If the drawing also calls for a decorative finish, the sequence matters — polishing after peening removes the very layer that was paid for.
2. Hertzian contact: the arithmetic of a single hit
For a sphere of radius R and mass m striking a flat at velocity v, the elastic impact solution gives the maximum indentation depth
the contact radius
and the peak contact pressure
where the combined modulus is
For steel on steel, E^* \approx 115 GPa. Take S230 shot: nominal diameter 0.58 mm, radius 0.29 mm, density 7,850 kg/m³, mass 0.80 mg. At 60 m/s:
The elastic pressure is absurd. A quenched and tempered steel with \sigma_y = 1.0 GPa flows at a contact pressure near 3\sigma_y = 3 GPa, so the real contact cannot reach 18 GPa. The contact becomes fully plastic, the pressure saturates near the hardness of the material, and the shot leaves a dimple whose depth is of the same order as the elastic deflection — 10–20 µm — with a surrounding lip of displaced metal.
This is the first reason not to treat peening as a pressure process. The peak pressure is set by the material's flow stress, not by the nozzle gauge. What the operator controls is the kinetic energy of the stream and the number of impacts per unit area. A bigger shot carries more energy at the same velocity (m \propto d^3), makes a wider and deeper dimple, and produces a deeper plastic zone. A faster shot carries more energy at the same size (E \propto v^2) and produces a more intense but not proportionally deeper layer.
Air-blast acceleration has its own ceiling. The air velocity in the nozzle chokes at the speed of sound, about 340 m/s at 20 °C, so increasing pressure above roughly 1.9 atm of pressure difference does not increase the air velocity — it increases the air density and therefore the mass flow. Shot velocities in air-blast systems typically reach 30–100 m/s; wheel-blast systems run higher. In one direct-pressure machine, ASR170 shot measured about 30 m/s at 0.14 MPa and 49 m/s at 0.35 MPa, following roughly v \propto p^{0.51} — a useful reminder that pressure-to-velocity is a machine-specific calibration, not a universal formula.
Stand-off distance is not arbitrary either. The shot accelerates in the expanding cone outside the nozzle, reaches a maximum velocity at some distance, then decelerates by drag. That maximum commonly falls around 200–250 mm for an air-blast nozzle. Peening too close gives an uneven, high-intensity footprint; peening too far gives a low, variable intensity. The Almen strip is how you find the actual window for your machine.
3. Almen intensity and the 10% rule
The Almen strip is a thin spring-steel coupon, 76.2 × 19.05 mm, clamped in a holder and peened on one side. When released, it bows toward the peened side. The arc height, measured on an Almen gauge, is the process response. Three thicknesses cover the useful range:
- N strip — 0.79 mm thick, for intensities below 0.10 mm A (0.004 in A), fine shot and low-energy processes.
- A strip — 1.29 mm thick, the reference strip, for 0.10–0.60 mm A (0.004–0.024 in A).
- C strip — 2.39 mm thick, for intensities above 0.60 mm A (0.024 in A), large shot and heavy sections.
A single strip does not give intensity. Intensity is defined from a saturation curve: peen strips at increasing exposure times with every other variable fixed, plot arc height against time, and find the point where doubling the exposure raises the arc height by no more than 10%. That point is T; the arc height at T is the intensity. SAE J443 (2025 revision) states the rule explicitly, and SAE J2597 covers computer-generated saturation curves.
The 10% rule looks arbitrary until you fit the curve. A saturating response is well approximated by
At the 10% point,
so
The “saturation” intensity is therefore about 90% of the theoretical asymptote, not 100%. Peening beyond T still adds arc height, but at less than 10% per doubling. That is why a strip exposed for 2T or 4T can read well above the intensity value without violating the specification: intensity is a property of the stream, not of how long one strip was exposed.
A worked curve makes the arithmetic concrete. Suppose four strips give 0.158 mm at 2 min, 0.216 mm at 4 min, 0.245 mm at 8 min, and 0.249 mm at 16 min. The curve is consistent with h_\infty = 0.25 mm and \tau = 2 min. Doubling from 4 min to 8 min raises the arc height by 13.4%; doubling from 8 min to 16 min raises it by 1.6%. The 10% crossing sits near 4.6 min at 0.225 mm, so the intensity is about 0.22 mm A, or 9A. The exact numbers depend on the strip lot, the holder, and the machine; the shape of the curve is the point.
Why the strip thickness changes the number
The arc height is not a direct readout of residual stress. For a peened layer of depth t and stress \sigma_c on a strip of thickness t_s, the bending moment per unit width is approximately M \approx \sigma_c t\,t_s/2, the curvature is \kappa = M/(EI), and with I = t_s^3/12,
Two consequences follow. First, arc height scales with 1/t_s^2, so a thinner strip bows far more for the same peening. The thickness-squared ratio between A and N is (1.29/0.79)^2 = 2.67, and the published rule of thumb is that the N strip reads about three times the A strip. Between C and A the ratio is (2.39/1.29)^2 = 3.43, and the published conversion is C × 3.5 ≈ A. The familiar conversion factors are not magic; they are the bending stiffness of the coupon.
Second, the strip is measuring a bending moment, not a stress. An 8A arc height is 0.203 mm, which corresponds to a curvature of 0.28 m⁻¹ and a radius of 3.6 m. The elastic bending strain at the strip surface is only 1.8 \times 10^{-4}, about 38 MPa of bending stress in the strip. The peened layer that produced it may be carrying 500–600 MPa over tens of micrometres. A 40 µm layer at 500 MPa on an A strip produces roughly 0.24 mm of arc height — the right order for 8–10A. The strip is a comparator, calibrated by history, not a stress sensor.
That is also why “8A” is not transferable between shot sizes. Eight thousandths on an A strip can be produced by fine shot at high velocity or coarse shot at low velocity. The arc heights match; the dimple sizes, the roughness, and the depth of the compressive layer do not. A drawing that specifies intensity without media size has specified only half the process.
4. Coverage: the Avrami arithmetic
Coverage is the fraction of the original surface that has been indented at least once. It is a statistical quantity, not a geometric one. If impacts arrive randomly at a constant rate \dot n per unit area and each makes a circular indent of radius r, the fraction of surface covered after time t follows the Avrami equation:
For practical inspection, 100% coverage is defined as 98% physical coverage — the point at which the remaining unpeened area is too small to see reliably under a magnifier. SAE J2277 is the coverage-determination standard. Setting C = 0.98,
So 98% coverage needs about four indent-areas of cumulative impact per unit area. “200% coverage” means peening for twice t_{98}, not covering 200% of the area. At twice the time, the physical coverage is
The extra time buys a process margin, not a second layer. On a manual operation, where nozzle angle and part rotation are operator-dependent, that margin matters: the 200% callout is a way of guaranteeing that no patch of surface is under-peened. On a well-controlled automatic machine, 100% is usually sufficient, and the second pass adds cost and surface damage without changing the residual-stress profile much.
A worked example shows how fast coverage accumulates. With S230 shot at 60 m/s, the dimple radius is about 72 µm (145 µm diameter). The indent area is 1.5 \times 10^{-8} m², so 98% coverage requires
At a mass flow of 5 kg/min, the stream delivers 1.04 \times 10^5 shots per second. Spread over a 100 cm² target, that is about 62,000 impacts/cm²/min, so 98% coverage takes about 25 s of perfect targeting — roughly a minute in a real cabinet with overspray and part geometry. The numbers are sensitive to shot size and flow: double the shot diameter and each impact covers four times the area, so the required impact count falls by four, but the mass flow for the same particle count also changes.
Coverage is also material-dependent. The Almen strip is spring steel at roughly 44–50 HRC. A soft aluminium part dimples more deeply and covers faster at the same stream; a hard gear covers more slowly. This is why coverage time must be established on the actual part material, not inferred from the Almen saturation time. The old practice of equating coverage time to Almen time is one of the most common specification errors.
5. The residual-stress profile, and how to measure it
The profile that matters is a function of depth, not a single number. It can be measured by X-ray diffraction using the \sin^2\psi method, by hole drilling per ASTM E837, by layer removal with strain gauges, or by neutron and synchrotron diffraction for thick sections. Each method has a different depth resolution and a different sensitivity to surface roughness; XRD sees the top 5–30 µm, hole drilling integrates through the drilled depth, and layer removal reconstructs the profile by progressively removing material.
The profile shape is set by the impact energy and the material. Higher intensity pushes the peak deeper and raises the surface compression, until the surface begins to damaged. The optimum is a balance: enough cold work to build a deep compressive layer, not so much that the surface develops laps, folds, or microcracks that become initiation sites.
Over-peening is real, and the gear data show it. In a study on a carburised helical gear with S230 shot, the mean fatigue life and B-10 life responded strongly to Almen intensity:
- Unpeened: mean 9,850 cycles, B-10 1,056 cycles.
- 12A: mean 16,571, B-10 7,708.
- 18A: mean 23,800, B-10 11,512.
- 24A: mean 33,167, B-10 11,953.
- 8C with S280 shot: mean 16,375, B-10 3,568.
The 24A condition more than tripled the mean life and raised B-10 by a factor of 11.3. The 8C condition, which is a coarser and more energetic stream, fell back to roughly the 12A mean and a B-10 of 3,568 — about one-third of the 24A B-10. The optimum was not the hardest stream the machine could produce; it was the stream that maximised the compressive layer while keeping surface damage below the initiation threshold.
The thermal limits are equally important. Residual stress relaxes by diffusion and creep, and the rate becomes significant above roughly 0.3–0.4 of the absolute melting temperature. In practice, aluminium alloys lose much of their peening benefit above about 120–150 °C, and steels above about 300–400 °C. A paint bake, a stress-relief cycle, or a hot straightening operation after peening can erase the layer. So can machining: grinding off 50 µm removes the peak of the profile and most of the benefit. Peening is a last-operation process, and the drawing should say so.
6. Media, machines, and the variables that actually move the result
The shot is the tool. SAE J444 defines cast-steel shot sizes from S110 (0.30 mm nominal) through S170 (0.43 mm), S230 (0.58 mm), S280 (0.71 mm), S330 (0.84 mm), S390 (1.0 mm), S460 (1.2 mm), S550 (1.4 mm), S660 (1.7 mm), S780 (2.0 mm), and S930 (2.4 mm). Cut-wire shot is available in the same nominal sizes with a more controlled roundness. Ceramic beads (zirconia or zirconia-silica) are used where iron contamination is unacceptable — titanium, aluminium, stainless steel — and glass beads are used for lower-intensity cosmetic or cleaning work.
Size selection follows a geometric rule: the shot should be no larger than about half the smallest fillet radius that must be peened. A 1.25 mm root radius calls for S230 at most; a 0.5 mm radius calls for S110 or S170. The same S230 shot has an effective intensity range of roughly 0.20–0.51 mm A on a typical machine, with a practical sweet spot around 0.25–0.46 mm A. Outside that range, the machine is either starved or the shot is being destroyed.
Hardness matters in both directions. For parts below about 50 HRC, cast-steel shot at 45–52 HRC is standard. Harder shot survives longer but can embrittle and fracture; softer shot deforms and loses roundness. Broken shot is worse than no shot: it cuts rather than peens, and the resulting surface is a stress raiser. Media condition is a control variable, not a consumable afterthought — screen for fines, check roundness, and add media on a schedule rather than when the stream looks thin.
The machine variables are interlocked:
- Air pressure changes mass flow and, to a lesser degree, shot velocity. It is not intensity.
- Media flow rate changes the number of impacts per second and therefore coverage time.
- Nozzle diameter changes the stream width and the air consumption.
- Stand-off changes both intensity and footprint; the maximum is usually 150–300 mm.
- Impingement angle changes the normal component of velocity. At 90° the full energy goes into the surface; at 45° only the normal component does, and the tangential component smears and roughens. Peening below about 30° is rarely useful.
- Part motion determines whether the coverage is uniform. A static nozzle shadows features; a robot or turntable is how complex parts get consistent coverage.
Masking is part of the process design. Threads, bearing bores, seal faces, splines, and precision fits are usually masked with rubber or polyurethane plugs and boots. Masking that slips during peening produces a part that is out of tolerance or has an unpeened patch — both are nonconformances. On a complex part, masking and handling can cost more than the peening itself.
7. Fatigue: what the layer buys, and when it does not
Fatigue cracks initiate at surfaces in tension. A compressive residual stress shifts the local mean stress negative, which reduces the effective stress intensity at the crack tip and delays both initiation and early growth. The simplest design picture is a Goodman-type superposition:
where \sigma_{res} is negative in compression. A −600 MPa residual in a 1,200 MPa steel can offset 600 MPa of tensile mean stress — a large fraction of the useful range. The benefit is largest for high-strength materials, notched parts, and surfaces that were previously in tension: ground, turned, EDM’d, or plated.
The data bear this out. For gear tooth root bending, a typical improvement in fatigue strength is 15–30%, with case-hardened gears benefiting more than through-hardened gears because the residual stress scales with the surface strength. For high-strength steel components generally, reported gains are several times in life at a given stress, or roughly 20–50% in fatigue strength. The gain is smallest on soft, ductile materials, where the compressive layer relaxes under load, and largest on hard, notched, or surface-damaged parts.
Two limits are often ignored:
Mean-stress limit. The benefit collapses as the applied maximum stress approaches tensile yield. The IIW recommendations for peened welds do not claim improvement above a stress ratio R > 0.5, and the benefit is reduced well before that. If the part yields on the first load cycle, the residual stress relaxes and the peening is gone.
Surface-quality limit. Peening roughens the surface. On a high-strength aluminium at high stress, that roughness can offset part of the residual-stress benefit. In one study on 7075-T6, shot peening increased fatigue life by about 1.6×, but polishing after peening raised it by about 3.4× — the roughness was a significant part of the result. If the design is roughness-sensitive, specify a light post-peen polish or a finer media, and remember that polishing removes some of the layer.
For welded joints, peening is a fatigue improvement technique in its own right. The IIW recommendations give a factor of 1.3 on stress range — about 2.2× on life for an S–N slope of 3 — for burr grinding, TIG dressing, or hammer/needle peening of low-strength steel; high-strength steel hammer-peened joints can claim 1.5× on stress range. Shot peening of welds is less effective than hammer peening because it does not modify the toe geometry as much: reported gains are around 30% in fatigue strength for shot-peened welds, versus 50–200% for hammer peening. On a weld, the geometry and the residual stress both matter, and the toe radius is usually the dominant notch.
8. Materials: the same process is not the same treatment
Steels. Cast-steel shot, 45–52 HRC, intensities from 6A to 12A, are the default for gears, springs, shafts, crankshafts, connecting rods, and bearing races. Case-hardened gears often use 8–12A with S230; heavy sections use S330 or S550 and C strips. Springs are peened after coiling and before preset; the compressive layer on the inside of the coil is what extends fatigue life.
Aluminium alloys. Steel shot can embed iron particles that become corrosion sites, especially on 2024 and 7075. Use ceramic or glass media, control the environment, and consider a post-peen cleaning step. Aluminium also has a lower melting point and a lower yield strength, so the residual stress relaxes at lower temperatures; a 120–150 °C bake can remove much of the benefit. Intensities are usually lower and N strips are common.
Titanium alloys. Iron contamination is unacceptable in aerospace titanium, so ceramic beads are the default. Ti-6Al-4V responds well to peening, but the surface must be clean and the media must be controlled. For additive titanium, peening is one of the few post-processes that addresses both the rough as-built surface and the tensile residual stress.
Stainless steels. Ceramic or glass media avoid free iron and the resulting pitting corrosion. Peening can improve fatigue and stress-corrosion resistance, but it can also smear surface defects if the media is contaminated. Cleanliness is part of the specification.
Nickel superalloys. IN718 and similar alloys are peened for fatigue and stress-corrosion resistance. Coverage matters, but the residual-stress profile is sensitive to the peening intensity and the subsequent heat treatment. One study found that even 20% coverage produced the same fatigue properties as 100% in IN718 — a reminder that the “100% minimum” rule is a process-control convention, not a law of physics, and that the optimum should be qualified on the actual alloy and geometry.
Additive manufacturing. As-built surfaces are rough, and the roughness is a crack initiator. HIP closes internal porosity but does not remove surface-connected defects or the rough surface, so HIP alone often does not restore fatigue life. Peening addresses both: it smooths the surface by plastic deformation and introduces compression. In EBM Ti-6Al-4V, ultrasonic shot peening raised the fatigue limit at 10^5 cycles from 220 MPa to 500 MPa, with surface residual stresses of −615 MPa longitudinal and −430 MPa transverse, a peak at about 30 µm and a layer that became insignificant beyond 300 µm. Shot peening improved the fatigue strength of DMLS and EBM Ti-6Al-4V by about 92–95% at 10^7 cycles in another study. What peening cannot do is heal a subsurface lack-of-fusion defect; if the defect is the initiation site, the surface treatment is irrelevant.
9. Peen forming: using the same stress to shape a part
If one side of a thin plate is peened, the plate bows toward the peened side. That is a distortion problem in fatigue peening and a manufacturing process in peen forming. The process was developed in the 1940s for integrally stiffened wing panels, patented by Lockheed in 1955, and is still used for wing skins, fuselage panels, and rocket structures. The lower wing panels of the A380 are a well-known example of pre-stress peen forming.
The mechanics are the same bending moment as the Almen strip, applied to a large panel. For a peened layer of depth t with an eigenstrain \varepsilon_p on a panel of thickness H, the curvature is approximately
For a 20 mm aluminium panel with a 0.3 mm layer at \varepsilon_p = 10^{-3}, \kappa = 4.5 \times 10^{-3}\ \text{m}^{-1}, a radius of about 222 m, and a sagitta of 0.51 m over a 30 m span. For a 3 mm sheet, the same layer gives a radius of about 5 m — which is why thin sheets distort so readily and why peen forming is a large-panel process, not a sheet-metal shortcut.
The process is controlled by intensity and coverage distribution, not by a single uniform pass. Chordwise curvature comes from peening one surface. Double curvature comes from pre-stressing the panel in a fixture and peening the tensile surface; the pre-stress can increase the forming limit by a factor of two to three. Edge peening on both sides adds length and helps produce saddle shapes. The shape is checked on a fixture, and the operator iterates: peen, measure, peen again. Accuracies of about 1 mm are achievable on panels up to 30 m long, but the iteration and the fixture are most of the cost.
Design rules follow from the mechanics. Avoid stiffeners parallel to the direction of curvature; avoid abrupt changes in thickness or curvature; design the part so that the peening can reach the surface; and remember that peen forming is a ductile-metal process — it does not apply to composites. For distortion correction, peening the concave side of a warped part can bring it back into tolerance without the marks of a press, which is why it is used on shafts, rings, and airframe components.
10. Specification and quality control on the shop floor
Shot peening is a special process: you cannot inspect the finished part to prove the layer is there without destroying it. You control the process, and you verify the process with Almen strips and coverage coupons. A complete drawing callout looks like this:
Peen per AMS 2430. Intensity 0.008–0.012A, 200% coverage, S230 cast-steel shot, 45–52 HRC. Peen all surfaces except masked threads, bores, and seal faces. Verify intensity with a saturation curve at the start of each shift and after any machine change. Do not machine, grind, or heat above 200 °C after peening.
The controls that matter:
- Almen strip lot and condition. Strips have thickness tolerances, pre-bow, and hardness requirements. A strip that is out of flatness or from an uncertified lot adds scatter that looks like process drift.
- Saturation curve. Build it per SAE J443 with at least four points, and keep the curve with the job. A single strip reading is not an intensity verification.
- Coverage coupon. Peen a representative coupon of the same material and inspect at 10–30×. For critical parts, use a fluorescent tracer or image analysis rather than a visual estimate.
- Media control. Check size, shape, hardness, and contamination. Broken shot and fines change the intensity and the surface finish.
- Machine parameters. Nozzle diameter, pressure, flow, stand-off, angle, and part motion should be recorded and locked. A robot program is a process specification.
- Masking. Verify that masks are seated, that they do not move during peening, and that they are removed before the next operation.
- Post-peening sequence. No machining, grinding, welding, or high-temperature bake after peening unless the drawing allows it.
AMS 2430 is the aerospace specification for automatic shot peening; AMS 2432 adds computer monitoring of the process variables; SAE J2441 is the general industry practice; Nadcap accreditation is common in aerospace supply chains. For general job-shop work, the same discipline can be applied with a written process sheet, a calibrated Almen gauge, and a saturation curve — the standard is a framework, not a substitute for understanding.
11. Economics: what the layer costs
Peening is cheap per square metre and expensive per part when masking and handling dominate. A transparent bottom-up model for an Indian job shop:
- Machine and operator: ₹1,200–2,500 per hour.
- Throughput: 5–20 m²/h for uniform coverage, depending on intensity, part geometry, and masking.
- Media: cast-steel shot at ₹80–150/kg, consumption 0.2–1 kg/h.
- Compressed air: 15–30 kW for a production cabinet, at ₹8/kWh.
At ₹1,500/h and 8 m²/h, machine time is about ₹190/m². Media adds ₹5–20/m², power ₹15–30/m², and masking and handling can add 30–100%. A realistic range for simple, unmasked parts is ₹200–400/m². A 0.02 m² bracket costs ₹4–8 in peening time, plus setup and inspection; a batch of 100 is a few hundred rupees. Peen forming is a different business: the value is in the fixture, the shape control, and the iteration, and the cost per square metre can be an order of magnitude or more above uniform fatigue peening.
The economics change the specification. Peening a non-cyclically loaded part buys nothing. Peening a part that will be machined after peening buys nothing. Peening at 200% coverage when 100% is qualified buys surface damage and time. The right question is not “what intensity is on the drawing?” but “what fatigue failure mode is this part exposed to, and what residual-stress profile addresses it?”
12. Alternatives and when to use them
Process · Typical depth · Surface effect · Best fit · Relative cost
Shot peening · 0.1–0.5 mm · Dimpled, cold-worked · Gears, springs, shafts, welds, AM · 1×
Laser shock peening · 1–2 mm · Minimal roughening · Fatigue-critical aero, holes, fillets · 5–20×
Ultrasonic impact / HFMI · 0.2–1 mm · Smoothed toe, deep compression · Weld toes, large structures · 2–5×
Cavitation peening · 0.1–0.5 mm · No media, complex geometry · AM titanium, internal surfaces · 3–10×
Low plasticity burnishing · 0.5–1 mm · Polished, low cold work · CNC-integrated critical surfaces · 5–15×
Hammer peening · 0.5–2 mm · Toe geometry modified · Weld toe repair, field work · Low, manual
Laser peening produces compression five to ten times deeper than shot peening with far less surface roughening, but it is line-of-sight, requires a sacrificial ablative layer, and costs much more per area. Ultrasonic impact treatment is the practical choice for weld toes on large structures: portable, deep, and backed by IIW design factors. Cavitation peening reaches internal surfaces and complex geometry without media, and has good data on additive titanium. Low plasticity burnishing is a CNC-integrated alternative that produces deep compression with minimal cold work, at a correspondingly higher cost.
None of these replaces the basic requirement: define the failure mode, qualify the process on the actual material and geometry, and control the variables that move the residual-stress profile.
FAQ
What does 8A mean in shot peening? 8A means an Almen intensity of 0.008 inch (0.203 mm) of arc height on an A strip, measured at the saturation point where doubling the exposure raises the arc height by 10% or less. It is a property of the shot stream, not a pressure or a direct stress value.
What is 200% coverage? 200% coverage means peening for twice the time needed to reach 100% coverage, where 100% is defined as 98% physical coverage. It is a time multiple, not twice the surface area; the physical coverage at 200% is about 99.96%, and the residual-stress profile is already close to saturated.
Does shot peening make a part stronger? It raises fatigue strength, fatigue life, and resistance to stress-corrosion cracking by introducing compressive residual stress. It does not increase static tensile strength, and it can reduce ductility and increase surface roughness.
How deep is the compressive layer? Typically 0.1–0.5 mm in steel, with the peak 20–75 µm below the surface. Laser peening reaches 1–2 mm, roughly five to ten times deeper. The depth depends on shot size, velocity, material, and intensity, not on the coverage alone.
Can I peen after machining or grinding? Yes — peening is normally the last mechanical operation. Do not machine, grind, or polish after peening unless the drawing allows it, because removing even 50 µm can remove the peak of the compressive layer.
What shot size should I use? Use shot no larger than about half the smallest fillet radius to be peened. S230 (0.58 mm) is common for gears and general steel parts; S110–S170 for small radii; S330–S550 for heavy sections; ceramic beads for titanium, aluminium, and stainless where iron contamination matters.
Why did my fatigue life get worse after peening? Over-peening is the usual cause: excessive intensity or coverage creates surface laps, folds, or microcracks that initiate fatigue. The gear data in this article show an 8C condition with a B-10 life one-third of the 24A optimum. Too-rough surfaces and peening before a machining operation are other common causes.
Does shot peening prevent corrosion? It improves resistance to stress-corrosion cracking and fretting, but it does not replace a coating or a corrosion-inhibiting primer. On stainless and titanium, iron contamination from steel shot can cause pitting, so ceramic or glass media are preferred.
Can you shot peen 3D-printed parts? Yes. Peening improves the fatigue strength of additive Ti-6Al-4V by roughly two times in published studies by smoothing the as-built surface and introducing compression. It cannot heal subsurface lack-of-fusion defects, which may still control fatigue life.
Is shot peening the same as sandblasting? No. Sandblasting uses angular abrasive media for cleaning or roughening and is not controlled by Almen intensity or coverage. Shot peening uses round media, controlled velocity, and a specified saturation curve to produce a defined compressive layer.
The short version
Shot peening is a fatigue process specified in arc height and time. A single S230 impact carries about 1.4 mJ, yields the surface at a contact pressure far above the elastic Hertz prediction, and leaves a dimple about 145 µm across. The useful result is a compressive layer 0.1–0.5 mm deep, peaking at 0.4–0.6 of the yield strength, which shifts the local mean stress negative and delays crack initiation.
Intensity is the arc height at the 10% saturation point, not a pressure. Coverage is the Avrami fraction of indented area, and 200% coverage is twice the time to 98%, not twice the area. The process window has an optimum: too little intensity leaves the layer shallow, too much damages the surface. The gear data make the penalty concrete — 24A more than tripled mean life, while 8C threw away two-thirds of the B-10 life that 24A delivered.
The shops that get peening right treat it as a controlled special process: qualified media, a saturation curve, coverage coupons, locked machine parameters, masking, and a sequence that puts peening last. The shops that get it wrong buy an Almen strip, hit the part until it looks matte, and wonder why the fatigue test scatters.